Shenzhen Alu Rapid Prototype Precision Co., Ltd.

Industry News

  • Home
  • News
  • Gate Freeze Time in Injection Molding: How to Set Holding Time

Gate Freeze Time in Injection Molding: How to Set Holding Time

Holding time in injection molding should not be chosen by habit or copied from a different mold. It should be long enough for holding pressure to compensate for material shrinkage until the gate seals, but not so long that the machine wastes cycle time after no more material can enter the cavity.

A gate-freeze study—also called a gate-seal study—is a practical way to identify that point. This guide explains how to run the study, interpret part weight and cavity-pressure data, and avoid common mistakes that produce misleading results.

What Happens During Packing and Holding?

After velocity-controlled filling, the machine transfers to pressure control. During packing and holding, pressure compresses the melt and pushes additional material into the cavity to compensate for volumetric contraction as the polymer cools.

Autodesk describes packing time and holding time as the same cycle stage and notes that the gate should freeze during this period. Once the gate freezes, the cavity is isolated from the runner. Continuing to apply holding pressure can no longer add material to the part.

Why Gate Freeze Time Matters

If holding time ends before gate seal, pressure in the cavity can fall too early and material may move back toward the runner. Possible results include:

  • Sink marks and internal voids

  • Low or inconsistent part weight

  • Dimensional instability

  • Excessive shrinkage

  • Warpage caused by uneven packing

  • Weakness in thick sections

If holding time continues well beyond gate freeze, part quality usually does not improve. The extra time increases cycle cost and may delay screw recovery, depending on machine sequence. The objective is a stable process with a small justified margin beyond the measured gate-seal point.

Gate Freeze Is Different From Part Cooling

Gate freeze time is not the same as cooling time or ejection time. The gate may seal while the center of a thick wall is still molten. Cooling must continue until the part has enough stiffness and dimensional stability for ejection.

BASF notes that the feed system and molding must be thermally balanced: a feed system that freezes too early prevents effective holding pressure, while one that freezes unnecessarily late can waste production time. The part wall near the gate has a strong influence on how long pressure can be transmitted.

Prepare the Process Before the Study

A gate-seal study is meaningful only after the basic process is stable. Before varying hold time, confirm:

  • Correct and consistently dried material

  • Stable melt and mold temperatures

  • Repeatable fill time and velocity-to-pressure transfer

  • A consistent melt cushion

  • A functioning nonreturn valve

  • Balanced cavity filling

  • Approved holding pressure

  • Consistent cooling time and cycle sequence

If fill volume, cushion, or check-ring behavior changes between shots, part weight can vary for reasons unrelated to gate freeze.

Run a Part-Weight Gate-Seal Study

The most common method is to mold parts at increasing holding times and weigh them after a consistent conditioning period.

  1. Establish a stable fill, transfer position, holding pressure, and cooling time.

  2. Begin with a short holding time that is known to be below gate freeze.

  3. Allow the process to stabilize after each setting change.

  4. Collect several consecutive parts from every cavity.

  5. Increase holding time in equal increments.

  6. Keep all other settings unchanged.

  7. Label parts by cavity, holding time, and shot sequence.

  8. Weigh parts on a suitable calibrated balance.

  9. Plot average part weight against holding time.

Autodesk and BASF both describe increasing holding time until part weight no longer changes. The beginning of the weight plateau indicates that additional holding time is no longer adding meaningful material through the gate.

Example of Interpreting the Weight Plateau

Suppose average part weight rises at 1, 2, 3, and 4 seconds of holding time, then remains essentially unchanged at 5, 6, and 7 seconds. This suggests that the gate seals around the transition into the plateau.

Do not select the first apparently flat point from one part. Review the measurement resolution, shot-to-shot variation, cavity differences, and whether the process was stable. Set production holding time slightly beyond the demonstrated seal point, using a margin appropriate to normal process variation.

Measure Each Cavity Separately

In a multi-cavity mold, combined shot weight can hide imbalance. One cavity may stop gaining weight while another continues. Weigh each cavity separately and plot independent curves.

Different freeze times can indicate:

  • Gate-size variation

  • Runner imbalance

  • Uneven mold temperature

  • Different cavity wall thickness

  • Vent or fill imbalance

  • Gate wear, damage, or partial blockage

The production holding time must support the latest required cavity, but large differences should trigger a mold-balance review rather than simply accepting a longer cycle.

Use Cavity Pressure When Available

Cavity-pressure sensors provide more direct evidence of pressure transmission and gate behavior. A post-gate sensor can show when pressure responds to holding and how the curve decays as the part cools. RJG notes that cavity-pressure curves can indicate gate seal and can reveal gate discharge or backflow.

Compare pressure curves across holding times. After the gate seals, extending machine hold should no longer change the relevant cavity-pressure response or part weight. Pressure data are especially valuable when weight differences are small, the resin absorbs moisture, or a multi-cavity tool is difficult to evaluate by combined weight.

Do Not Confuse Holding Time With Holding Pressure

A long holding time cannot compensate for pressure that is too low or blocked by a frozen flow path. Likewise, excessive holding pressure can create:

  • Flash

  • Overpacked regions near the gate

  • High molded-in stress

  • Part sticking or difficult ejection

  • Gate-area stress and cracking

  • Uneven shrinkage and warpage

Develop holding pressure and holding time as related but separate process variables. First establish a stable fill and transfer; then choose a pressure profile that produces acceptable packing; finally confirm the time required to reach gate seal.

Check the Melt Cushion and Nonreturn Valve

The screw must retain a consistent cushion so the machine can apply pressure without bottoming out. If the cushion reaches zero, the machine cannot transmit the commanded holding pressure correctly. If cushion varies widely, suspect inconsistent dosing, leakage across the nonreturn valve, or material feeding problems.

BASF lists lack of melt cushion and nonreturn-valve problems among conditions that can prevent adequate shrinkage compensation. Record cushion position with each study point.

How Gate Design Affects Freeze Time

Gate thickness, width, length, type, and location determine how quickly the gate cools. A small gate may seal before a thick section is adequately packed. A very large gate can extend freeze time and leave a larger vestige or increase cycle time.

Autodesk recommends gating into a thicker region where practical because this helps maintain filling and packing paths. A thin section between the gate and a thick feature may freeze first and isolate the thick region even when the gate itself remains open.

Hot runners and valve gates require special interpretation. Valve closure can mechanically isolate the cavity before natural thermal freeze. Study the actual production sequence, including valve timing, pressure response, and possible gate discharge.

Material and Temperature Effects

Gate-freeze time changes with resin, additives, moisture, melt temperature, mold temperature, and thermal properties. Higher melt or mold temperature often delays freeze, while lower temperature may shorten the open time. Semi-crystalline and amorphous materials also solidify differently.

Run the study with approved production material and temperature settings. If the process has a wide validated temperature window, confirm that the selected holding time remains adequate at the condition most likely to delay or advance gate seal.

Common Gate-Seal Study Mistakes

  • Changing holding pressure and holding time at the same time

  • Using combined shot weight for an imbalanced multi-cavity mold

  • Collecting only one part per setting

  • Ignoring unstable melt cushion or check-ring leakage

  • Changing settings before the process reaches stability

  • Weighing hygroscopic parts after inconsistent conditioning

  • Using a balance with insufficient resolution

  • Assuming a flat curve means the thickest region is properly packed

  • Confusing gate freeze with safe ejection time

  • Setting hold exactly at the estimated freeze point with no margin

Gate Freeze Study Checklist

  • Record material lot, drying, melt temperature, and mold temperature.

  • Verify fill time, transfer point, cushion, and nonreturn-valve repeatability.

  • Hold pressure, cooling time, and other variables constant.

  • Increase holding time in controlled increments.

  • Collect multiple stable shots at each setting.

  • Identify and weigh every cavity separately.

  • Plot weight against holding time and review variation.

  • Review cavity-pressure curves when sensors are available.

  • Confirm sink, dimensions, warpage, flash, and ejection quality.

  • Document the selected time and its process margin.

Information to Send for an Injection Mold Review

For troubleshooting or mold quotation, provide the 3D model, 2D drawing, resin grade, wall-thickness map, gate and runner layout, cavity count, machine data, current process sheet, part weights by cavity, defect photographs, and cavity-pressure traces if available.

Aluprototype supports injection mold DFM, gate and runner review, mold manufacturing, process development, trial molding, and dimensional inspection. Send us your project data for a practical molding review and quotation.

References